Aluminium Anodizing Umusaruro Wibisobanuro

Aluminium Anodizing Umusaruro Wibisobanuro

Inzira

1.Gukoresha ibikoresho bishingiye kuri feza hamwe nibikoresho bya elegitoroniki ya elegitoronike: Gutwara - Gukaraba Amazi - Gukonjesha ubushyuhe buke - Gukaraba amazi - Gukaraba Amazi - Gufata - Anodizing - Gukaraba Amazi - Gukaraba Amazi - Gukaraba Amazi - Kwoza Amazi - Gukaraba Amazi - Kwoza amazi - Guhumeka - Kuma ikirere - Kugenzura - Kwinjira muri electrophoreis - Gupakira.

2.Gukoresha ibikoresho bikonje hamwe nibikoresho bya electrophoreque bikonje: Kuzamura - Kugabanuka - Gukaraba Amazi - Gukata Acide - Gukaraba Amazi - Gukaraba Amazi - Gukaraba Amazi - Gukaraba Amazi - Gukaraba Amazi - Kutabogama no Kuzimya - Gukaraba Amazi - Kwoza Amazi - Gukomeretsa - Anodizing - Kwoza Amazi - Kwoza Amazi - Kwoza Amazi - Gufunga umwobo - Gukaraba Amazi - Gukaraba Amazi - Guhumeka - Kuma ikirere - Kugenzura - Kwinjira muri electrophoreis - Gupakira.

3.Guhindura ibikoresho byamabara hamwe nibikoresho byamabara ya electrophoreque: Gutwara - Gukaraba Amazi - Gukonjesha Ubushyuhe Buke - Gukaraba Amazi - Gukaraba Amazi - Gufata - Anodizing - Gukaraba Amazi - Gukaraba Amazi - Gukaraba Amazi - Gukaraba - Gukaraba Amazi - Gukaraba Amazi - Gufunga Amazi - Kwoza amazi - Kwoza amazi - Kugenzura - Kwinjira muri electrophoreis - Guhisha - Kuma ikirere - Kugenzura - Gupakira.蓝色氧化

Anodizing ibicuruzwa bya MAT Aluminium

Gutwara Ibikoresho

1.Mbere yo gupakira imyirondoro, isura yo guhuza inkoni yo guterura igomba guhanagurwa neza, kandi gupakira bigomba gukorwa ukurikije umubare usanzwe. Inzira yo kubara niyi ikurikira: Umubare wimyirondoro yapakiwe = Ubucucike bugezweho x Umwanya umwe wumwirondoro.

2.Amahame yo gusuzuma umubare wa racks: Igipimo cyo gukoresha ubushobozi bwimashini ya silicon ntigomba kurenga 95%; ubucucike buriho bugomba gushyirwaho 1.0-1.2 A / dm; imiterere yumwirondoro igomba gusiga icyuho gikenewe hagati yimyirondoro ibiri.

3.Kubara igihe cya anodizing: Anodizing time (t) = Ubunini bwa firime burigihe K x Ubucucike bwa k, aho K ni electrolysis ihoraho, ifatwa nka 0.26-0.32, na t iri muminota.

4.Iyo gupakira ibice byo hejuru, umubare wumwirondoro ugomba gukurikiza imbonerahamwe ya "Umwanya wumwirondoro numubare wa Racks yo hejuru".

5.Kworohereza amazi na gazi, ibice byo hejuru bigomba kugororwa mugihe cyo guhuza, hamwe nu mpande zingana na dogere 5.

6.Inkoni iyobora irashobora kwaguka kurenza umwirondoro wa 10-20mm kumpande zombi, ariko ntigomba kurenza 50mm.

Ubushyuhe buke bwo gutunganya

1.Ubushuhe bwibikoresho byogeza ubushyuhe buke muri tank bigomba kugenzurwa kuri acide yuzuye ya 25-30 g / l, byibuze 15 g / l.

2.Ubushyuhe bwikigega gisya bugomba kubikwa kuri 20-30 ° C, byibuze byibuze 20 ° C. Igihe cyo gusya kigomba kuba amasegonda 90-200.

3.Nyuma yo guterura no gukuramo amazi asigaye, imyirondoro igomba kwimurwa vuba mumazi wamazi kugirango yoge. Nyuma yo koza amazi abiri, agomba guhita yimurirwa mu kigega cya anodizing. Igihe cyo gutura mu kigega cy'amazi ntigishobora kurenza iminota 3.

4. Mbere yo gusya, ibikoresho byo hasi yubushyuhe buke ntibigomba gukorerwa ubundi buvuzi, kandi andi mazi ya tank ntagomba kwinjizwa mumatara.

Gutesha agaciro inzira

1.Ibikorwa byo gutesha agaciro bikorwa mugisubizo cya acide mubushyuhe bwicyumba, hamwe niminota 2-4 hamwe na H2SO4 yibanda kuri 140-160 g / l.

2.Nyuma yo guterura no gukuramo amazi asigaye, imyirondoro igomba gushyirwa mumazi wamazi kugirango yoze muminota 1-2.

Ubukonje (Acide Etching) Inzira

1.Nyuma yo kwangirika, imyirondoro igomba kwozwa mumazi mbere yo kwinjira mukigega cya acide.

2.Ibipimo bitunganyirizwa: NH4HF4 yibanze kuri 30-35 g / l, ubushyuhe bwa 35-40 ° C, pH agaciro ka 2.8-3.2, nigihe cyo gufata aside muminota 3-5.

3.Nyuma ya acide, imyirondoro igomba kunyura mumazi abiri mbere yo kwinjira mukigega cya alkali.

Inzira ya Alkali

1.Ibipimo bitunganijwe: Ubushuhe bwa NaOH bwubusa bwa 30-45 g / l, ubwinshi bwa alkali ya 50-60 g / l, umuti wa alkali wa 5-10 g / l, AL3 + ubunini bwa 0-15 g / l, ubushyuhe bwa 35-45 ° C, hamwe na alkali igihe cyo gufata ibikoresho byumucanga byamasegonda 30-60.

2.Nyuma yo guterura no gukuramo igisubizo, imyirondoro igomba kwimurwa vuba mumazi wamazi kugirango yoze neza.

3.Ubuziranenge bwubuso bugomba kugenzurwa nyuma yo gukora isuku kugirango hamenyekane ko nta kimenyetso kibora, umwanda, cyangwa gufatira hejuru mbere yo kwinjira muburyo bwo kumurika.

Kumurika

1.Ibipimo bitunganijwe: H2SO4 yibanze kuri 160-220 g / l, HNO3 muburyo bukwiye cyangwa 50-100 g / l, ubushyuhe bwicyumba, nigihe cyo kumurika cyiminota 2-4.

2.Nyuma yo guterura no gukuramo amazi asigaye, imyirondoro igomba kwimurwa vuba mumazi wamazi muminota 1-2, hagakurikiraho ikigega cya kabiri cyamazi muminota 1-2.

3.Nyuma yibice bibiri byogusukura, insinga ya aluminiyumu kumurongo igomba gufatanwa neza kugirango hamenyekane neza mugihe cya anodizing. Ibikoresho bisanzwe bifatanyirizwa kumutwe umwe wumugozi wa aluminiyumu ya rack, mugihe ibikoresho byamabara nibikoresho bya electrophoreque bifatanye kumpande zombi.

Inzira ya Anodizing

1.Ibipimo bitunganijwe: Ubushuhe bwa H2SO4 bwa 160-175 g / l, AL3 + kwibanda ≤20 g / l, ubucucike bwa 1-1.5 A / dm, voltage ya 12-16V, ubushyuhe bwa anodizing ya 18-22 ° C. Igihe cyo gukwirakwiza amashanyarazi kibarwa ukoresheje formulaire. firime isabwa: ibikoresho bya feza 3-4 mm, umucanga wera 4-5 mm, electrophoreis 7-9μm;

2.Ibice bya anode bigomba gushyirwa mu ntebe ziyobora, kandi bigomba kwemezwa ko ntaho bihurira na profili na plaque ya cathode mbere yo gutangira inzira ya anodizing.

3.Nyuma ya anodizing, inkoni ya anode igomba gukurwa mumazi, kugoreka, no kuvoma amazi asigaye. Hanyuma bagomba kwimurirwa mu kigega cyamazi kugirango bakarabe muminota 2.

4.Imiterere idafite amabara irashobora kwinjira mumazi ya kabiri yo kuvura kashe.

Amabara

1.Ibara ryibara rigomba gutondekwa gusa kumurongo umwe wumurongo wikubye kabiri, hamwe nintera iri hagati yibicuruzwa bingana cyangwa birenze ubugari bwisura bwibicuruzwa byegeranye. Mubisanzwe, iyo bipimye n'intoki, intera igomba kuba irenze cyangwa ingana n'ubugari bw'intoki ebyiri. Bundles zigomba kuba zifunze kandi zifite umutekano, kandi imirongo mishya igomba gukoreshwa muguhuza.

2.Ubushyuhe bwa anodizing mugihe cyo kurangi bigomba kugenzurwa kuri 18-22 ° C kugirango uburebure bwa firime imwe kandi nziza.

3.Ibice byamabara anodize muri buri murongo bigomba kuba bingana.

4.Nyuma yo kurangi, imyirondoro igomba guhindagurika, ugereranije nurubaho rwamabara, kandi niba ibisabwa byujujwe, birashobora kwozwa mumazi. Bitabaye ibyo, hagomba gufatwa ingamba zihariye.

5.Ni byiza kwirinda amabara yubwoko butandukanye bwibicuruzwa cyangwa ibyiciro bitandukanye byibicuruzwa kumurongo umwe.

 aluminium

Anodizing ibicuruzwa bya MAT Aluminium

Uburyo bwo gushiraho ikimenyetso,

1. Shira imyirondoro ya anodize mu kigega gifunga kugirango ufunge firime ya anodize kandi wongere imbaraga zo kurwanya ruswa ya firime.

2.Ibipimo bitunganijwe: Ubushyuhe busanzwe bwo gufunga ubushyuhe bwa 10-30 ° C, igihe cyo gufunga iminota 3-10, pH agaciro ka 5.5-6.5, icyuma cya kashe ya 5-8 g / l, nikel ion ya 0.8-1.3 g / l, hamwe na fluoride ion yibanda kuri 0.35-0.8 g / l.

3.Nyuma yo gufunga, uzamure ibisate, uhengamye kandi unyunyuze amazi ya kashe, ubyohereze mumazi wamazi kugirango woge kabiri (umunota 1 buri mwanya), uhumure umwirondoro, ubikure kumurongo, ubigenzure kandi byumishe mbere yo gupakira. .

Byahinduwe na Gicurasi Jiang wo muri MAT Aluminium


Igihe cyo kohereza: Ukwakira-21-2023